Dielectrical Constants of Polymers
Compound |
ε (Exper.) |
ε (Calc.) |
Polyacetal, Poly(methylene oxide), POM |
3.0 |
3.0 |
Poly(acrylonitrile), PAN |
3.2 |
3.1 |
Poly(Bisphenol A carbonate), PC |
3.0 |
3.1 |
Poly(1,4-butadiene), PBD |
2.5 |
2.3 |
Poly(1-butene), PB-1 |
2.3 |
2.2 |
Poly(butyl methacrylate), PBMA |
2.8 |
2.7 |
Poly(caprolactam), PA 6 |
4.1 |
4.0 |
Poly(caprolactone), PCL |
|
2.9 |
Poly(2-chloro-p-xylylene) |
3.0 |
2.8 |
Poly(2-chlorostyrene) |
2.8 |
2.8 |
Poly(4-chlorostyrene) |
2.7 |
2.8 |
Poly(chlorotrifluoroethylene) |
2.6 |
2.6 |
Poly(cyclohexyl methacrylate), PCHMA |
2.6 |
2.7 |
Poly(2,6-dimethyl-p-phenylene oxide), PPI |
2.7 |
2.7 |
Poly(2,6-diphenyl-p-phenylene oxide) |
2.8 |
2.8 |
Poly(ethyl methacrylate), PEMA |
2.9 |
2.9 |
Poly(ethylene terephthalate), PET |
3.4 |
3.5 |
Poly(ethylene), PE |
2.2 |
2.2 |
Poly(isobutene) |
2.2 |
2.2 |
Poly(isobutyl methacrylate) |
2.7 |
2.7 |
Poly(isobutylethylene) |
2.1 |
2.2 |
Poly(methyl methacrylate), PMMA |
3.0 |
3.0 |
Poly(2-methylstyrene) |
2.5 |
2.5 |
Poly(4-methylstyrene), PMS, PPMS |
2.5 |
2.5 |
Poly(1,4-phenyl ether) , PPE |
2.6 |
2.9 |
Poly(propylene glycol), PPG |
|
2.5 |
Poly(propylene), PP |
2.2 |
2.2 |
Poly(p-xylene) |
2.7 |
2.6 |
Poly(thio-1,4-phenylene), PPS |
3.1 |
3.0 |
Poly(α-methylstyrene) , PαMS |
2.6 |
2.5 |
Poly[(tetramethylene terephthalate), PBT |
3.2 |
3.2 |
Poly{[bis(4-chlorophenyl)sulfone]-alt-[bisphenol-A]}, PSU |
3.3 |
3.1 |
Polyhexamethylene adipamide, PA 6,6 |
4.0 |
4.0 |
Polyhexamethylene sebacamide, PA 6,10 |
3.6 |
3.5 |
Polystyrene, PS |
2.5 |
2.6 |
Polytetrafluoroethylene, Teflon, PTFE |
2.0 |
2.0 |
Polytetrahydrofuran, PTMO |
|
2.5 |
Poly(vinyl acetate), PVAc, PVA |
3.2 |
3.2 |
Polyvinyl chloride, PVC |
3.1 |
3.0 |
Polyvinyl fluoride, PVF |
|
2.1 |
Polyvinylidene chloride, PVDC |
2.9 |
|
Polyvinylidene fluorid, PVDF |
|
2.0 |